Process Hierarchy

  Silicon nitride LPCVD
Process characteristics:
Thickness
Amount of material added to a wafer
Thickness*
Amount of material added to a wafer, must be 0 .. 1.2 µm
0 .. 1.2 µm
Ambient
Ambient to which substrate is exposed during processing
nitrogen
Batch size 24
Deposition rate
Rate at which material is added to a wafer
0.0045 µm/min
Material silicon nitride
Pressure
Pressure of process chamber during processing
0.048 kPa
Residual stress 1250 MPa
Sides processed both
Temperature 810 .. 830 °C
Wafer size
Wafer size
Equipment Thermco TMX furnace (C-stack, tube #4)
Equipment characteristics:
Wafer holder
Device that holds the wafers during processing.
quartz boat
Wafer materials
List of wafer materials this tool can accept (not list of all materials, just the wafer itself).
silicon
Wafer thickness
List or range of wafer thicknesses the tool can accept
300 .. 800 µm
Comments:
  • Index of refraction = 1.98
    Uniformity ~ 2.6%