on front Aluminum plasma etch |
|
Process characteristics: |
Depth Depth of material removed by etch process |
|
Ambient Ambient to which substrate is exposed during processing |
boron trichloride, chlorine, nitrogen, sulfur hexafluoride |
Batch size |
4 |
Etch rate |
0.6 µm/min |
Loading effects Free form text field for description of loading effects (e.g. bullseye) |
Highly sensitive |
Material |
aluminum |
Min feature size |
1 µm |
Pressure Pressure of process chamber during processing |
200 mTorr |
Selectivity Primary material removal rate divided by removal rates of secondary materials (i.e., factors by which primary material is removed faster than secondary materials) |
aluminum: 1, photoresist (category): 1.5, silicon dioxide: 6 |
Sides processed |
either |
Temperature |
80 °C |
Wafer size |
|
Equipment |
Applied Materials Precision 5000 (chamber A) |
Equipment characteristics: |
Wafer holder Device that holds the wafers during processing. |
mechanical clamp |
Wafer materials List of wafer materials this tool can accept (not list of all materials, just the wafer itself). |
silicon, quartz (single crystal), silicon on insulator, silicon germanium |
Wafer thickness List or range of wafer thicknesses the tool can accept |
400 .. 750 µm |
Comments: |
|